Skip to main content
HuntHumber

2026-10-15 · 2 min read · Panel Bonding Resins

Reading a peel test on an aluminium composite panel

Two panels can give the same peel force and fail in different layers. The force trace and the fracture surfaces belong in the same test record.

What the peel arm contributes

Kendall peeled rubber from glass at different angles and separated the work of creating a new surface from the work of stretching the rubber. The elastic contribution became important at shallow angles. Aluminium skins can also bend permanently. The experiment explains why geometry matters, but its elastic model cannot supply an acceptance value for a metal panel.

Source · K. Kendall (1975), Thin-film peeling—the elastic term

Follow the fracture across the strip

Mark the start and direction of the peel before testing. Match a stable length of the force trace to the same length on both fracture surfaces. Exposed metal, adhesive on both faces and torn core point to different fracture paths. A strip that tears through the core gives limited information about the strength of the metal interface.

Make an ageing comparison interpretable

Cut adjacent strips from one panel. Keep one as a control and condition the other under the agreed exposure. Match skin gauge, strip width, peel angle, speed and specimen temperature. Report force per unit width together with the failure location. A shift from core tearing to separation at the metal surface merits investigation even when the mean force changes little.